GARBAFLEX 11R51
Flat and shaped wire
GARBAFLEX 11R51 is an austenitic stainless steel wire alloyed with molybdenum, supplied in the cold rolled or annealed condition.
C (%) | Si (%) | Mn (%) | P max. (%) | S max. (%) | Cr (%) | Ni (%) | Mo (%) |
---|---|---|---|---|---|---|---|
0.07 - 0.09 | 1.20 - 1.80 | 1.50 - 2.00 | 0.025 | 0.010 | 16.00 - 18.00 | 7.00 - 8.50 | 0.50 - 0.80 |
Tensile strength
As cold rolled max. 2400 N/mm2.
As annealed max. 850 N/mm2.
For flat rolled wire
Width (mm) | Tolerance (mm) |
---|---|
1.00 - 5.00 | ±0.050 |
5.01 - 8.00 | ±0.070 |
8.01 - 10.00 | ±0.100 |
Thickness (mm) | Tolerance (mm) |
---|---|
0.30 - 0.80 | ±0.015 |
0.81 - 1.00 | ±0.019 |
1.01 - 1.60 | ±0.025 |
For shaped wire
Width (mm) | Tolerance (mm) |
---|---|
1.50 | ±0.020 |
1.51 - 3.00 | ±0.030 |
3.01 - 5.00 | ±0.040 |
5.01 - 7.00 | ±0.050 |
7.01 | ±0.060 |
Elongation
As annealed min. 40%.
Microstructure
Austenite.
Execution
Rolled on 2 sides (flat).
Rolled on 4 sides (shaped).
Camber
Max. 3 mm measured on 1 m length.
Surface
Bright. Surface defects max. 1% of thickness.
E and G modulus of elasticity
Abt. 180 kN/mm2 in drawn condition.
Abt. 185 kN/mm2 after heat treatment.
E and G modulus of shear
Abt. 70 kN/mm2 in drawn condition.
Abt. 73 kN/mm2 after heat treatment.
Density: 7.90 kg/dm3.
Additional information
Delivery form
On wooden spools, max. 250 kg.